Effect of thermomechanical aging on force system of orthodontic aligners made of different thermoformed materials: An in vitro study
Tarek M. Elshazly, Ludger Keilig, Diva Nang, Bijan Golkhani, Anna K. Weber, Hanaa Mohamed Samir Elattar et al. · 2024 · 11 citationsRead the paper
PURPOSE: The aim was to investigate the effect of aging by thermocycling and mechanical loading on forces and moments generated by orthodontic clear aligners made from different thermoplastic materials. METHODS: A total of 25 thermoformed aligners made from 5 different materials, i.e., Essix ACE® and Essix® PLUS™ (Dentsply Sirona, Bensheim, Germany), Invisalign® (Align Technology, San Jose, CA, USA), Duran®+ (Iserlohn, Germany), Zendura™ (Fremont, CA, USA), underwent a 14-day aging protocol involving mechanical loading (a 0.2 mm vestibular malalignment of the upper left second premolar [tooth 25]) and thermocycling in deionized water (temperature range 5-55 °C). The 3D forces/moments exerted on tooth 25 of a resin model were measured at three time points: before aging (day 0), after 2 days and after 14 days of aging. RESULTS: Before aging, extrusion-intrusion forces were 0.6-3.0 N, orovestibular forces were 1.7-2.3 N, and moments as mesiodistal rotation were 0.3-42.1 Nmm. In all directions, multilayer Invisalign® exhibited the lowest force/moment magnitudes. After aging, all materials showed a significant force/moment decay within the first 2 days, except Invisalign® for orovestibular and vertical translation. However, following thermomechanical aging, Duran®+ and Zendura™ aligners had equivalent or even higher vestibular forces (direction of mechanical load). CONCLUSION: Thermomechanical aging significantly reduced forces and moments during the first 48 h. Multilayer aligner materials exhibit lower initial forces and moments than single-layer ones, and were less influenced by aging. Material hardening was observed after subjecting some of the aligner materials to mechanical loading. Thus, orthodontists should be aware of possible deterioration of orthodontic aligners over time. This work also sheds light on how material selection impacts the mechanical behavior of aligners and may provide valuable guidance regarding optimal timing for the aligner changing protocol.
What the full text shows
Shown in the lab- Significant force and moment decay occurred within the first 48 hours of thermomechanical aging across almost all materials. — Significant drop within 2 days; no further significant drop from day 2 to 14 (14-day aging protocol (thermocycling 5-55 °C and 0.2 mm mechanical loading))
- Multilayer materials (Invisalign) produced significantly lower initial forces and moments and were less affected by aging than single-layer materials. — Lowest force/moment magnitudes among all tested materials (Initial state and post-aging)
- Initial extrusion-intrusion forces ranged from 0.6 to 3.0 N, and orovestibular forces from 1.7 to 2.3 N. — 0.6-3.0 N (vertical), 1.7-2.3 N (orovestibular) (Before aging (Day 0))
- Initial moments for distal rotation were significantly higher than for mesial rotation. — 23.1-42.1 Nmm (distal) vs 0.3-14.2 Nmm (mesial) (Before aging (Day 0))
- Certain materials exhibited hardening (increased stiffness) after mechanical loading. — Increase in vestibular forces after 14 days (Specifically observed for Duran+)
- Setup
- 25 aligners (n=5 per material: Essix ACE, Essix PLUS, Invisalign, Duran+, Zendura) on 3D-printed resin models.
- How
- Five thermoplastic materials were thermoformed into aligners and subjected to a 14-day aging protocol of thermocycling (5-55 °C) and mechanical loading (0.2 mm malalignment). 3D forces and moments were measured using a custom-made biomechanical device (OMSS) at day 0, 2, and 14.
- Limitations
- Used deionized water instead of artificial saliva due to device limitations. · In vitro study lacks the cushioning effect of the periodontal ligament (PDL). · Small sample size (n=5 per group).
Summarized by Gemma 4 from the open-access full text · 16 Nov 2026. Read it